What is RAFT?

RAFT (Reversible Addition-Fragmentation chain Transfer) is a form of living radical polymerization involving conventional free radical polymerization of a substituted monomer in the presence of a suitable chain transfer (RAFT) reagent. Use of the appropriate RAFT agent and polymerization conditions allows for the synthesis of polymers with low PDI and high functionality.  

Reagents

Reagents

Loading

Precautions and Disclaimer

These products are for R&D use only, not for drug, household, or other uses. Please consult the Safety Data Sheet for information regarding hazards and safe handling practices.

Storage/Stability

723274 - Store the product at –20 °C and keep tightly closed. The product is light sensitive.

722995 and 723037 - Store the products at 2–8 °C and keep tightly closed.

722987723002723010, and 723029 - Store the products at 2–8 °C and keep tightly closed. The products are light sensitive.

Procedures

Procedures of RAFT polymerization as performed by researchers at CSIRO.

Methyl Methacrylate Polymerization

Uses methyl methacrylate (MMA, Catalog Number M55909) as the monomer, AIBN (Catalog Number 441090) as the initiator, and a RAFT agent (Catalog Number 722987 or 723274).

  1. Prepare stock solution of methyl methacrylate (15 mL, 0.14 mol) and AIBN (20.1 mg, 0.122 mmol) in 5 mL of benzene.
  2. Aliquot 2 mL samples of stock solution into ampules containing Catalog Number 722987 (12.3 mg, 0.056 mmol) or Catalog Number 723274 (22.5 mg, 0.056 mmol). Note: Other glassware suitable for handling air sensitive reactions, such as a schlenk reaction tube (Catalog Number Z515981), may be used as an alternative to a sealed ampule.
  3. De-gas contents of ampules by three repeated freeze-evacuate-thaw cycles (0.05 mmHg) and seal under vacuum.
  4. Polymerize by placing sealed ampule in heated oil bath (60 °C) for 15 hours.

Researchers at CSIRO have tested select RAFT agents in the polymerization of methyl methacrylate and analyzed the resulting polymers. The data are presented in Table 1.

NMR of poly methyl methacrylate

Figure 1.NMR of poly(methyl methacrylate) polymerized for 15 hours using Catalog Number 722987 as a RAFT agent

Vinyl Acetate Polymerization

Uses vinyl acetate (Catalog Number V1503) as the monomer, AIBN (Catalog Number 441090) as the initiator, and a RAFT agent (Catalog Number 723002).

  1. Prepare solution of vinyl acetate (2.0 mL, 23.23 mmol), AIBN (2.0 mg, 0.012 mmol), and Catalog Number 723002 (26.64 mg, 0.12 mmol) in an ampule. Note: Other glassware suitable for handling air sensitive reactions, such as a schlenk reaction tube (Catalog Number Z515981), may be used as an alternative to a sealed ampule.
  2. De-gas contents of the ampule by three repeated freeze-evacuate-thaw cycles (0.05 mm Hg) and seal under vacuum.
  3. Polymerize by placing sealed ampule in heated oil bath (60 °C) for 16 hours.

Researchers at CSIRO have tested select RAFT agents in the polymerization of vinyl acetate and analyzed the resulting polymer. The data are presented in Table 2.

GPC analysis

Figure 2.GPC analysis of poly(vinyl acetate) polymerized for 16 hours using Catalog Number 723002 as a RAFT agent

Materials

Loading

Patents WO98/01478 and WO99/311444